Round robin prueba el análisis XRF XRF EQAS St Gobain - SGIC, Vidrio borosilicato
VAT No.:
San Gobain Isover - CRIR
Material de comparación entre laboratorios:
SGIC, vidrio borosilicato
Estudio terminado:
2002 - 6
Bibliografía:
Informe final
elementos principales [wt %]
| CRB | RV | 1sRV | Z-Score | |
| Na₂O | 16,800 | 16,820 | 0,165 | --- |
| MgO | 2,520 | 2,610 | 0,060 | --- |
| Al₂O₃ | 1,200 | 1,490 | 0,070 | --- |
| SiO₂ | 63,870 | 64,050 | 0,310 | --- |
| P₂O5 | 0,153 | 0,150 | 0,014 | --- |
| SO₃ | 0,200 | 0,190 | 0,030 | --- |
| K₂O | 0,480 | 0,048 | 0,020 | --- |
| CaO | 7,890 | 7,850 | 0,110 | --- |
| TiO₂ | 0,069 | 0,070 | 0,013 | --- |
| Fe₂O₃ tot. | 0,390 | 0,410 | 0,020 | --- |
| MnO | 0,235 | 0,240 | 0,018 | --- |
oligoelementos [µg/g]
| CRB | RV | 1sRV | Z-Score | |
| Ba | 300,00 | --- | --- | --- |
| Rb | 60,00 | --- | --- | --- |
| Sr | 320,00 | --- | --- | --- |
| Zr | 280,00 | --- | --- | --- |
Leyenda
CRB
resultados CRB
essai interlaboratorios
Resultados del estudio colaborativo
1s-RV
Estudio colaborativo de desviación estándar
Z-Score
Diferencia entre el valor medido y el estudio promedio
*